Xi’an Hitachi 63 type dry capacitor box welding

1. The difficulties in the welding process are as follows:

Box main weld size control

Box weld size requirements: x:0-1mm y:0-1.5mm

Back penetration size: 0-1mm

The box weld adopts pulse MIG welding, the outer and inner dimensions of the weld are in conflict with each other due to the influence of welding heat input, the welding heat input is too large, the outer weld is too small, and the back penetration size is easy to exceed the difference. The welding heat input is too small, the back penetration size is too small, and the outer weld size is out of tolerance. In order to achieve both sides of the weld size and meet the requirements. It is necessary to find a suitable balance value within a small adjustable range of parameters.

Appearance requirements for main weld of box body

The appearance quality of the main welds on the enclosure is subject to extremely stringent requirements. Due to production volume and efficiency demands, fully automated mechanized welding is employed. The enclosure is assembled from L‑shaped and U‑shaped bent components, with lap joints as the weld configuration; the lap width is 0.6–0.8 mm, resulting in narrow weld beads. To achieve efficient, high-quality automated welding, the stability of the welding power source, the precision of the robotic arm, and the coordination between welding speed, wire feed rate, and welding parameters all require precise adjustment.

Control of Lifting Lug Weld Size and Post-Weld Flatness

The box hanging climbing weld adopts manual TIG welding. The weld joint is a 4mm aluminum plate and a 2mm aluminum plate T-shaped double-sided fillet weld. The weld length is relatively short, and the protrusion on the back of the 2mm thin plate weld shall not exceed 0.5mm. After welding, the flatness is required to be controlled within 1mm. Therefore, the technical requirements for manual TIG welding welders are high. At the same time, in order to control the deformation of the 2mm thin plate after welding, the welding process needs internal support and speed up the heat dissipation.

Appearance Requirements for Hanging and Climbing Welds

The appearance of the main weld of the box body is required to be high. Manual TIG welding is adopted. The weld joint is a T-shaped double-sided fillet weld of 4mm aluminum plate and 2mm aluminum plate, and the weld length is short. And the back of the weld is strictly prohibited from welding through, requiring extremely high manual welding skills for welders.

Appearance requirements for suspension welds

The appearance of the box is extremely high, and there shall be no obvious appearance defects such as scratches, bumps, oil stains, etc. The material of the box body is aluminum plate, and the oxide layer on the surface is extremely fragile. It is very easy to cause scratches and bumps during the loading and unloading of the welding process and the circulation of each process. Therefore, the protection requirements for the surface of the aluminum plate are very high in each process.

2. The following are the measures to address the difficulties in the welding process.

1) Control measures for main weld size and appearance of box body

Make special welding clamping tooling, press the outside of the weld area, and use chrome zirconium copper C1 chamfer support block to form a welding pad on the back to support the molten pool to limit the penetration size of the weld back. The welding process parameter test is carried out to compare the influence ability of each parameter on the weld size, and finally control and adjust the balance one by one, so as to realize the synchronization of the outer and inner dimensions of the weld to meet the requirements.

2) Hanging and climbing weld size and appearance control measures

Special tooling for hanging and climbing welding is made. The back of the 2mm plate of the box body is supported by copper plate. During the welding process, the heat dissipation of the aluminum plate is accelerated and the welding deformation is controlled. The tooling is rotated by a single-axis positing machine to realize the flat fillet welding position where all 4mm thick plates are located on the bottom surface, and the heat is concentrated on the thick plates to prevent the thin plates from being welded through. Through cross dislocation welding, the single position welding heat input is reduced, and the flatness of the sheet surface after welding is controlled. The welding test plate is used to strengthen the welding training of welders for such welds, improve the welding stability, and adjust the appropriate welding parameters according to the welding rate of each welder’s personal habit. Ensure that the weld is stably formed and has no obvious defects in appearance.

3) Overall appearance control measures

The protective film of the non-welding area of the raw material shall be retained throughout the whole process. Wear protective gloves during all operation steps. Bare hands are prohibited. Material transfer must use special pallets/shelves

Welding seam spatter, welding slag, scratches, bumps and oil stains shall be locally polished with special tools and standard mesh gas grinding plates.